[Skip to Content](https://www.sigmaaldrich.com#main-content) [![Merck](https://www.sigmaaldrich.com/static/logos/purple/merck.svg)](https://www.sigmaaldrich.com/CZ/en) Products Cart0 CZEN Products ProductsApplicationsServicesResourcesSupport [Login / Register](https://www.sigmaaldrich.com/oidc-sign-in) [Order Lookup](https://www.sigmaaldrich.com/CZ/en/order-lookup) [Quick Order](https://www.sigmaaldrich.com/CZ/en/quick-order) Cart0 [Home](https://www.sigmaaldrich.com/CZ/en)[Organic Electronics](https://www.sigmaaldrich.com/CZ/en/applications/materials-science-and-engineering/organic-electronics)Procedure for Standard Surface Modification using the Aldrich® Kit for Creating Hydrophilic PDMS Surfaces # Procedure for Standard Surface Modification using the Aldrich® Kit for Creating Hydrophilic PDMS Surfaces ## Product Description Use of this kit results in a durable hydrophilic PDMS surface. The resulting surface should be wettable by hydrophilic inks and appropriate for multiple printing applications. After treatment, water should completely wet the surface as the water contact angle is expected to be between 25 and 35 °. ## Components Solution A - 10 mL (Glycidyl methacrylate based polymer) Solution B - 4 mL (Acrylamide/acrylic acid based polymer) ## Solvents recommended, but not provided 1. Ethanol (Catalog Number __245119__) 2. 2-Butanone (Catalog Number __230294__) 3. Water (Catalog Number __320072__) ## Precautions and Disclaimer This product is for R&D use only, not for drug, household, or other uses. Please consult the Safety Data Sheet for information regarding hazards and safe handling practices. ## Storage/Stability Store the kit at room temperature. ## Procedure Procedure for standard surface modification ![Procedure for standard surface modification](https://www.sigmaaldrich.com/content/dam/cms-commons/sigmaaldrich/marketing/global/images/technical-documents/protocols/materials-science-and-engineering/organic-electronics/procedure-for-standard-a.gif "Procedure for standard surface modification") 1. Pretreatment - PDMS surface should be activated using a low frequency air plasma treatment for 1 minute (Recommended plasma cleaners: Catalog Numbers __Z561673__, __Z561681__, __Z561657__, and __Z561665__). 2. Prerinsing - The plasma activated PDMS sample should be rinsed by washing with ethanol (Catalog Number __245119__) for at least 10 minutes. The rinsing procedure should be repeated 3 times. Then, the sample should be air-dried for at least 15 minutes. The water contact angle of the resulting activated PDMS surface is expected to be between 25 and 40 °C. 3. First Modification Step - The surface of the horizontally positioned sample prepared in the previous step should be covered with Solution A, typically ~1 mL per square inch of the surface. The sample should be dried under ambient conditions for 20–30 minutes and annealed at 110 °C under nitrogen or argon for 30 minutes. 4. Rinsing - The annealed sample should be rinsed three times with 2-Butanone (Catalog Number __230294__) for 10 minutes each time. Then it should be air-dried for at least 30 minutes. 5. Polymer Grafting - 6 mL of ethanol must be added to the container containing Solution B. Stir the mixture to homogeneity. The surface of the horizontally positioned sample prepared previously should be treated by completely covering the area to be modified with the homogeneous solution, typically ~1 mL per square inch of the surface. The sample should be dried under ambient conditions for 20–30 minutes, then annealed at 80 °C for 14 hours. Finally, the unattached polymer should be removed from the sample by a thorough rinse with water (Catalog Number __320072__) and the sample air-dried at room temperature. ## Materials Sorry, an unexpected error has occurred Response not successful: Received status code 500 __Related Articles__ - [Kit for Creating Hydrophilic PDMS Surfaces](https://www.sigmaaldrich.com/CZ/en/technical-documents/protocol/materials-science-and-engineering/organic-electronics/kit-for-creating-hydrophilic) - [Preparing Self-Assembled Monolayers](https://www.sigmaaldrich.com/CZ/en/technical-documents/protocol/materials-science-and-engineering/organic-electronics/preparing-self-assembled) - [Thioacetate Deprotection Procedure](https://www.sigmaaldrich.com/CZ/en/technical-documents/protocol/materials-science-and-engineering/organic-electronics/thioacetate-deprotection) Top __Sign In To Continue__ To continue reading please sign in or create an account. Sign In__Don't Have An Account?__Register Support[Customer Support](https://www.sigmaaldrich.com/CZ/en/support/customer-support)[Contact Us](https://www.sigmaaldrich.com/CZ/en/collections/offices)[FAQ](https://maestro.my.site.com/knowledgeportal/s/)[Safety Data Sheets (SDS)](https://www.sigmaaldrich.com/CZ/en/documents-search?tab=sds)[Certificates (COA/COO)](https://www.sigmaaldrich.com/CZ/en/documents-search?tab=coa)[Quality & Regulatory](https://www.sigmaaldrich.com/CZ/en/life-science/quality-and-regulatory-management)[Calculators & Apps](https://www.sigmaaldrich.com/CZ/en/support/calculators-and-apps)[Webinars](https://www.sigmaaldrich.com/CZ/en/collections/webinars) Orders[Order Lookup](https://www.sigmaaldrich.com/CZ/en/order-lookup)[Quick Order](https://www.sigmaaldrich.com/CZ/en/quick-order)[Custom Products](https://www.sigmaaldrich.com/CZ/en/services/custom-products)[eCommerce Solutions](https://www.sigmaaldrich.com/CZ/en/life-science/ecommerce/ecommerce-solutions) Company[About Us](https://www.sigmaaldrich.com/CZ/en/life-science/about-us)[Responsibility](https://www.sigmaaldrich.com/CZ/en/life-science/ssbi)[Events](https://www.sigmaaldrich.com/CZ/en/collections/events)[Press Releases](https://www.sigmaaldrich.com/CZ/en/collections/press)[Programs](https://www.sigmaaldrich.com/CZ/en/life-science/partnership-programs)[Careers](https://careers.merckgroup.com/global/en)[Offices](https://www.sigmaaldrich.com/CZ/en/collections/offices) Social Media [![LinkedIn icon](https://www.sigmaaldrich.com/content/dam/cms-commons/sigmaaldrich/marketing/global/images/icons/linkedin.svg)](https://www.linkedin.com/company/merck-life-science) [![X icon](https://www.sigmaaldrich.com/content/dam/cms-commons/sigmaaldrich/marketing/global/images/icons/x-icon.svg)](https://x.com/Merck_lifesci) [![Facebook Icon](https://www.sigmaaldrich.com/content/dam/cms-commons/sigmaaldrich/marketing/global/images/icons/facebook.svg)](https://www.facebook.com/Merck.lifescience) [![Instagram Icon](https://www.sigmaaldrich.com/content/dam/cms-commons/sigmaaldrich/marketing/global/images/icons/instagram.svg)](https://www.instagram.com/mercklifescience/) [![YouTube Icon](https://www.sigmaaldrich.com/content/dam/cms-commons/sigmaaldrich/marketing/global/images/icons/youtube.svg)](https://www.youtube.com/@MerckLifeScience/featured) Merck __Research. Development. Production.__ We are a leading supplier to the global Life Science industry with solutions and services for research, biotechnology development and production, and pharmaceutical drug therapy development and production. [![Vibrant M string](https://www.sigmaaldrich.com/content/dam/cms-commons/sigmaaldrich/marketing/global/images/icons/vibrant-m-string-1-rrvcrp.svg)](https://www.sigmaaldrich.com/CZ/en) [Sigma-Aldrich® Solutions](https://www.sigmaaldrich.com/CZ/en/life-science/sigma-aldrich)[BioReliance® Solutions](https://www.sigmaaldrich.com/CZ/en/life-science/bioreliance)[Millipore® Solutions](https://www.sigmaaldrich.com/CZ/en/life-science/millipore)[SAFC® Solutions](https://www.sigmaaldrich.com/CZ/en/life-science/safc)[Milli-Q® Solutions](https://www.sigmaaldrich.com/CZ/en/life-science/milliq)[Supelco® Solutions](https://www.sigmaaldrich.com/CZ/en/life-science/supelco) © 2026 Merck KGaA, Darmstadt, Germany and/or its affiliates. All Rights Reserved, including Text and Data Mining for AI training and similar technologies. Reproduction of any materials from the site is strictly forbidden without permission. [Site Use Terms](https://www.sigmaaldrich.com/CZ/en/life-science/legal/site-use-terms)|[Privacy Policy](https://www.sigmaaldrich.com/CZ/en/life-science/legal/privacy-statement)|[General Terms and Conditions of Sale](https://www.sigmaaldrich.com/CZ/en/life-science/legal/terms-and-conditions)|[Copyright Consent](https://www.sigmaaldrich.com/CZ/en/life-science/legal/copyright-consent) |[Site Map](https://www.sigmaaldrich.com/CZ/en/site-map) An unknown error has occured.