[跳轉至內容](https://www.sigmaaldrich.com#main-content)
[](https://www.sigmaaldrich.com/TW/zh)
產品
購物車0
TWZH
產品
產品應用服務資源支援
[登入 / 註冊](https://www.sigmaaldrich.com/oidc-sign-in)
[訂單查詢](https://www.sigmaaldrich.com/TW/zh/order-lookup)
[快速下訂](https://www.sigmaaldrich.com/TW/zh/quick-order)
購物車0
[Home](https://www.sigmaaldrich.com/TW/en)[Microelectronics & Nanoelectronics](https://www.sigmaaldrich.com/TW/en/applications/materials-science-and-engineering/microelectronics-and-nanoelectronics)Kit for PDMS Surface Modification
# Kit for PDMS Surface Modification
[Materials](https://www.sigmaaldrich.com#materials)
In collaboration with Clemson University and the Pennsylvania State University, we have developed a [Surface Modification Kit](https://www.sigmaaldrich.com/TW/en/product/aldrich/701912), which allows for durable hydrophilization of various polydimethylsiloxane (PDMS) surfaces.
The procedure is based on technology developed by the group of Professor I. Luzinov (Clemson University). It employs a macromolecular anchoring layer approach for grafting hydrophilic polymer layers onto hydrophobic PDMS surfaces.
One of the possible applications for hydrophilic PDMS surfaces is microcontact printing. Figure 1 compares hydrophilic ink imprints, which have been created using untreated, oxygen plasma treated and kit modified PDMS surfaces.

Untreated PDMS surface

Oxygen plasma treated PDMS surface: 1st imprint

Oxygen plasma treated PDMS surface: 4th imprint

Kit modified PDMS surface: 1st imprint

Kit modified PDMS surface: 10th imprint
__Figure 1__. Imprints of a hydrophilic electroceramic ink on metal substrate created using differently treated PDMS surfaces. (Courtesy of Professor Susan Trolier-McKinstry, the Pennsylvania State University)
Technical facts and applications of this technology can be found in the following publications:
- Zdyrko, B.; Klep, V.; Luzinov, I. *Material Matters*, 2008, *3(2)*, 44.
- Nagata, S.H.; Ko, S.W.; Hong, E.; Randall, C.A.; Trolier-McKinstry, S. *J. Am. Ceram. Soc.*, 2006, *89*, 2816.
- Nie, Z.; Kumacheva, E. *Nature Materials*, 2008, *7(4)*, 277.
## Surface Modification Kit
Product No. [701912](https://www.sigmaaldrich.com/TW/en/product/aldrich/701912)
__Kit Components__
Solution A (Glycidyl methacrylate based polymer) 10 mL
Solution B (Acrylamide/acrylic acid based polymer) 4 mL
Recommended Solvents (not included)
- Ethanol (Product No. [270741](https://www.sigmaaldrich.com/TW/en/product/sigald/270741))
- 2-Butanone (Product No. [34861](https://www.sigmaaldrich.com/TW/en/product/sigald/34861))
- Water (Product No. [320072](https://www.sigmaaldrich.com/TW/en/product/sigald/320072))

__Figure 2.__Schematic of the PDMS surface hydrophilization process.
### Procedure
1. __Pretreatment__ - PDMS surface should be activated using a low frequency air plasma treatment for 1 minute (Recommended plasma cleaners: Product Nos. [Z561673](https://www.sigmaaldrich.com/TW/en/product/aldrich/Z561673), [Z561681](https://www.sigmaaldrich.com/TW/en/product/aldrich/Z561681), [Z561657](https://www.sigmaaldrich.com/TW/en/product/aldrich/Z561657), and [Z561665](https://www.sigmaaldrich.com/TW/en/product/ALDRICH/Z561665)).
2. __Prerinsing__ - The plasma activated PDMS sample should be rinsed by washing with ethanol (Product No. [270741](https://www.sigmaaldrich.com/TW/en/product/sigald/270741)) for at least 10 minutes. The rinsing procedure should be repeated 3 times. Then, the sample should be air-dried for at least 15 minutes. The water contact angle of the resulting activated PDMS surface is expected to be between 25 and 40°.
3. __First Modification Step__ - The surface of the horizontally positioned sample prepared in the previous step should be covered with Solution A, typically ~1 mL per square inch of the surface. The sample should be dried under ambient conditions for 20–30 minutes and annealed at 110 °C under nitrogen or argon for 30 minutes.
4. __Rinsing__ - The annealed sample should be rinsed three times with 2-Butanone (Product No. [34861](https://www.sigmaaldrich.com/TW/en/product/sigald/34861)) for 10 minutes each time. Then it should be air-dried for at least 30 minutes.
5. __Polymer Grafting__ - 6 mL of ethanol must be added to the container containing Solution B. Stir the mixture to homogeneity. The surface of the horizontally positioned sample prepared previously should be treated by completely covering the area to be modified with the homogeneous solution, typically ~1 mL per square inch of the surface. The sample should be dried under ambient conditions for 20–30 minutes, then annealed at 80 °C for 14 hours. Finally, the unattached polymer should be removed from the sample by a thorough rinse with water (Product No. [320072](https://www.sigmaaldrich.com/TW/en/product/sigald/320072)) and the sample air-dried at room temperature.
After treatment, water should effectively wet the surface as the water contact angle is expected to be between 25 and 35°. The resulting PDMS surface should be wettable by hydrophilic inks and appropriate for multiple printing applications.
## Materials
抱歉,發生意外錯誤。
Response not successful: Received status code 500
__Related Articles__
- [AISF: A Solid Alternative to Sulfuryl Fluoride Gas](https://www.sigmaaldrich.com/TW/en/technical-documents/technical-article/chemistry-and-synthesis/fluorination/stable-alternative-aisf)
- [Atomic Layer Deposition of Nanomaterials for Li-Ion Batteries, Fuel Cells, and Solar Cells](https://www.sigmaaldrich.com/TW/en/technical-documents/technical-article/materials-science-and-engineering/batteries-supercapacitors-and-fuel-cells/atomic-layer-deposition-of-nanomaterials-for-li-ion-batteries-fu)
- [Carbon Nanofiber Applications & Properties](https://www.sigmaaldrich.com/TW/en/technical-documents/technical-article/materials-science-and-engineering/batteries-supercapacitors-and-fuel-cells/carbon-nanofibers)
- [Graphene in Biotechnology](https://www.sigmaaldrich.com/TW/en/technical-documents/technical-article/materials-science-and-engineering/bioelectronics/graphene-in-biotechnology)
- [Electronic and Biomedical Applications of High-Purity Single-Walled Nanotubes (SWNTs)](https://www.sigmaaldrich.com/TW/en/technical-documents/technical-article/materials-science-and-engineering/bioelectronics/nanointegris)
- [Nature as the Source of Materials for More Sustainable Organic Electronics](https://www.sigmaaldrich.com/TW/en/technical-documents/technical-article/materials-science-and-engineering/bioelectronics/nature-as-source-of-materials-for-more-sustainable-organic-electronics)
- [Substrate and Conductor Materials Towards More Sustainable Electronics](https://www.sigmaaldrich.com/TW/en/technical-documents/technical-article/materials-science-and-engineering/bioelectronics/substrate-and-conductor-materials-towards-more-sustainable-electronics)
- [Graphene Quantum Dots: Properties, Synthesis & Applications](https://www.sigmaaldrich.com/TW/en/technical-documents/technical-article/materials-science-and-engineering/biosensors-and-imaging/graphene-quantum-dots)
- [View More](https://www.sigmaaldrich.com/TW/en/search/facet-search?focus=sitecontent&term=facet-search)
頂部
__登入以繼續__
若要繼續閱讀,請登入或建立帳戶。
登入__還沒有帳戶?__註冊
支援[客戶支援](https://www.sigmaaldrich.com/TW/zh/support/customer-support)[聯絡我們](https://www.sigmaaldrich.com/TW/zh/collections/offices)[常見問題](https://maestro.my.site.com/knowledgeportal/s/)[安全資料表 (SDS)](https://www.sigmaaldrich.com/TW/zh/documents-search?tab=sds)[證書 (COA/COO)](https://www.sigmaaldrich.com/TW/zh/documents-search?tab=coa)[品質與法規](https://www.sigmaaldrich.com/TW/zh/life-science/quality-and-regulatory-management)[計算機與應用程式](https://www.sigmaaldrich.com/TW/zh/support/calculators-and-apps)[網路研討會](https://www.sigmaaldrich.com/TW/zh/collections/webinars)
訂單[訂單查詢](https://www.sigmaaldrich.com/TW/zh/order-lookup)[快速訂購](https://www.sigmaaldrich.com/TW/zh/quick-order)[客製化產品](https://www.sigmaaldrich.com/TW/zh/services/custom-products)[電子商務解決方案](https://www.sigmaaldrich.com/TW/zh/life-science/ecommerce/ecommerce-solutions)
公司簡介[關於我們](https://www.sigmaaldrich.com/TW/zh/life-science/about-us)[責任](https://www.sigmaaldrich.com/TW/zh/life-science/ssbi)[活動](https://www.sigmaaldrich.com/TW/zh/collections/events)[新聞稿](https://www.sigmaaldrich.com/TW/zh/collections/press)[節目](https://www.sigmaaldrich.com/TW/zh/life-science/partnership-programs)[工作機會](https://careers.merckgroup.com/global/en)[辦公室](https://www.sigmaaldrich.com/TW/zh/collections/offices)
社交媒體
[](https://www.linkedin.com/company/merck-life-science)
[](https://x.com/Merck_lifesci)
[](https://www.facebook.com/Merck.lifescience)
[](https://www.instagram.com/mercklifescience/)
[](https://www.youtube.com/@MerckLifeScience/featured)
Merck
__Research.開發。生產。__
我們是全球生命科學產業的領導供應商,提供研究、生物技術開發與生產,以及藥物治療開發與生產的解決方案與服務。
[](https://www.sigmaaldrich.com/TW/zh)
[Sigma-Aldrich® 溶液](https://www.sigmaaldrich.com/TW/zh/life-science/sigma-aldrich)[BioReliance® 解決方案](https://www.sigmaaldrich.com/TW/zh/life-science/bioreliance)[Millipore® 溶液](https://www.sigmaaldrich.com/TW/zh/life-science/millipore)[SAFC® 解決方案](https://www.sigmaaldrich.com/TW/zh/life-science/safc)[Milli-Q® 解決方案](https://www.sigmaaldrich.com/TW/zh/life-science/milliq)[Supelco® 解決方案](https://www.sigmaaldrich.com/TW/zh/life-science/supelco)
© 2026 Merck KGaA, Darmstadt, Germany 和/或其附屬公司。版權所有,包括用於 AI 訓練的文字和資料挖掘以及類似技術。
未經許可,嚴禁複製本網站的任何資料。
[網站使用條款](https://www.sigmaaldrich.com/TW/zh/life-science/legal/site-use-terms)|[隱私權政策](https://www.sigmaaldrich.com/TW/zh/life-science/legal/privacy-statement)|[一般銷售條款](https://www.sigmaaldrich.com/TW/zh/life-science/legal/terms-and-conditions)|[版權同意書](https://www.sigmaaldrich.com/TW/zh/life-science/legal/copyright-consent)|[網站地圖](https://www.sigmaaldrich.com/TW/zh/site-map)